AISI 4340 Steel, oil quenched 855°C (1570°F), 230°C (450°F) temper for 4 hrs., tested at 26°C
Subcategory: AISI 4000 Series Steel; Ferrous Metal; Low Alloy Steel; Medium Carbon Steel; Metal
Key Words: alloy steels, UNS G43400, AMS 5331, AMS 6359, AMS 6414, AMS 6415, ASTM A322, ASTM A331, ASTM A505, ASTM A519, ASTM A547, ASTM A646, MIL SPEC MIL-S-16974, B.S. 817 M 40 (UK), SAE J404, SAE J412, SAE J770, DIN 1.6565, JIS SNCM 8, IS 1570 40Ni2Cr1Mo28, IS 1570 40NiCr1Mo15
Component | Wt. % |  | | C | 0.37 - 0.43 | | Cr | 0.7 - 0.9 | | Fe | 96 | |
| Component | Wt. % |  | | Mn | 0.7 | | Mo | 0.2 - 0.3 | | Ni | 1.83 | |
| Component | Wt. % |  | | P | Max 0.035 | | S | Max 0.04 | | Si | 0.23 | |
|
Physical Properties | Metric | English | Comments |
|
Density | 7.85 g/cc | 0.284 lb/in³ | |
Mechanical Properties |
|
Hardness, Knoop | 555 | 555 | Converted from Vickers hardness. |
Hardness, Vickers | 531 | 531 | |
Tensile Strength, Ultimate | 1855 MPa | 269000 psi | |
Tensile Strength, Yield | 1550 MPa | 225000 psi | |
Elongation at Break | 12 % | 12 % | |
Reduction of Area | 40 % | 40 % | |
Modulus of Elasticity | 196 GPa | 28400 ksi | |
Bulk Modulus | 140 GPa | 20300 ksi | Typical for steel. |
Poisson's Ratio | 0.3 | 0.3 | Calculated |
Machinability | 50 % | 50 % | annealed and cold drawn. Based on 100% machinability for AISI 1212 steel. |
Shear Modulus | 75 GPa | 10900 ksi | Estimated from elastic modulus |
Electrical Properties |
|
Electrical Resistivity | 2.48e-005 ohm-cm | 2.48e-005 ohm-cm | 20°C (68°F) |
Electrical Resistivity at Elevated Temperature | 2.98e-005 ohm-cm | 2.98e-005 ohm-cm | 100°C (212°F) |
Electrical Resistivity at Elevated Temperature | 5.52e-005 ohm-cm | 5.52e-005 ohm-cm | 400°C (750°F) |
Electrical Resistivity at Elevated Temperature | 7.97e-005 ohm-cm | 7.97e-005 ohm-cm | 600°C (1110°F) |
Thermal Properties |
|
CTE, linear 20°C | 12.3 µm/m-°C | 6.83 µin/in-°F | specimen oil hardened, 600°C (1110°F) temper; 20-100°C (68-212°F) |
CTE, linear 20°C | 12.7 µm/m-°C | 7.06 µin/in-°F | specimen oil hardened, 600°C (1110°F) temper; 20-200°C (68-390°F) |
CTE, linear 250°C | 12.6 µm/m-°C | 7 µin/in-°F | 1.88% Ni, normalized, tempered; 21-260°C (70-500°F) |
CTE, linear 250°C | 13.7 µm/m-°C | 7.61 µin/in-°F | specimen oil hardened, 600°C (1110°F) temper; 20-400°C (68-750°F) |
CTE, linear 500°C | 13.7 µm/m-°C | 7.61 µin/in-°F | 1.88% Ni, normalized and tempered; 21-540°C (70-1000°F) |
CTE, linear 500°C | 13.9 µm/m-°C | 7.72 µin/in-°F | 1.90% Ni, quenched, tempered; 21-540°C (70-1000°F) |
CTE, linear 500°C | 14.5 µm/m-°C | 8.06 µin/in-°F | specimen oil hardened, 600°C (1110°F) temper; 20-600°C (68-1110°F) |
Specific Heat Capacity | 0.475 J/g-°C | 0.114 BTU/lb-°F | Typical 4000 series steel |
Thermal Conductivity | 44.5 W/m-K | 309 BTU-in/hr-ft²-°F | Typical steel |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|