AISI 4340 Steel, oil quenched 830°C (1525°F), 540°C (1000°F) temper, nitrided


Subcategory: AISI 4000 Series Steel; Ferrous Metal; Low Alloy Steel; Medium Carbon Steel; Metal

Key Words: alloy steels, UNS G43400, AMS 5331, AMS 6359, AMS 6414, AMS 6415, ASTM A322, ASTM A331, ASTM A505, ASTM A519, ASTM A547, ASTM A646, MIL SPEC MIL-S-16974, B.S. 817 M 40 (UK), SAE J404, SAE J412, SAE J770, DIN 1.6565, JIS SNCM 8, IS 1570 40Ni2Cr1Mo28, IS 1570 40NiCr1Mo15

Component   Wt. %
C0.37 - 0.43 
Cr0.7 - 0.9 
Fe96 
Component   Wt. %
Mn0.7 
Mo0.2 - 0.3 
Ni1.83 
Component   Wt. %
PMax 0.035 
SMax 0.04 
Si0.23 

Material Notes:
Specimens nitrided at 525°C for 48 hrs. True fatigue limit: R.R. Moore rotating beam fatigue specimens with min. diameter of 5.84 mm, 0.25 mm root-radius notch 0.51 mm deep. Normalized at 940 - 955°C.

Physical PropertiesMetricEnglishComments
Density7.85 g/cc0.284 lb/in³ 

Mechanical Properties
Hardness, Knoop335335 Converted from Rockwell C hardness.
Hardness, Rockwell C3333 core hardness
Hardness, Vickers323323 Converted from Rockwell C hardness.
Modulus of Elasticity205 GPa29700 ksi Typical for steel
Bulk Modulus140 GPa20300 ksi Typical for steel.
Poisson's Ratio0.290.29 Calculated
Machinability50 %50 % annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus80 GPa11600 ksi Typical for steel.

Electrical Properties
Electrical Resistivity2.48e-005 ohm-cm2.48e-005 ohm-cm 20°C (68°F)
Electrical Resistivity at Elevated Temperature2.98e-005 ohm-cm2.98e-005 ohm-cm 100°C (212°F)
Electrical Resistivity at Elevated Temperature5.52e-005 ohm-cm5.52e-005 ohm-cm 400°C (750°F)
Electrical Resistivity at Elevated Temperature7.97e-005 ohm-cm7.97e-005 ohm-cm 600°C (1110°F)

Thermal Properties
CTE, linear 20°C12.3 µm/m-°C6.83 µin/in-°F specimen oil hardened, 600°C (1110°F) temper; 20-100°C (68-212°F)
CTE, linear 20°C12.7 µm/m-°C7.06 µin/in-°F specimen oil hardened, 600°C (1110°F) temper; 20-200°C (68-390°F)
CTE, linear 250°C12.6 µm/m-°C7 µin/in-°F 1.88% Ni, normalized, tempered; 21-260°C (70-500°F)
CTE, linear 250°C13.7 µm/m-°C7.61 µin/in-°F specimen oil hardened, 600°C (1110°F) temper; 20-400°C (68-750°F)
CTE, linear 500°C13.7 µm/m-°C7.61 µin/in-°F 1.88% Ni, normalized and tempered; 21-540°C (70-1000°F)
CTE, linear 500°C13.9 µm/m-°C7.72 µin/in-°F 1.90% Ni, quenched, tempered; 21-540°C (70-1000°F)
CTE, linear 500°C14.5 µm/m-°C8.06 µin/in-°F specimen oil hardened, 600°C (1110°F) temper; 20-600°C (68-1110°F)
Specific Heat Capacity0.475 J/g-°C0.114 BTU/lb-°F Typical 4000 series steel
Thermal Conductivity44.5 W/m-K309 BTU-in/hr-ft²-°F Typical steel

References for this datasheet.


Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistant format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. MatWeb data and tools provided by MatWeb, LLC.