AISI Type 314 Stainless Steel, annealed bar
Subcategory: Ferrous Metal; Metal; Stainless Steel; T 300 Series Stainless Steel
| Component | Wt. % |  | | | C | 0.25 | | | Cr | Max 26 | | | Fe | 47 | | | Mn | 2 | | | Ni | Max 22 | | | P | 0.045 | | | S | 0.03 | | | Si | Max 3 | |
|
| Physical Properties | Metric | English | Comments |
|
| Density | 7.8 g/cc | 0.282 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 180 | 180 | |
| Hardness, Knoop | 201 | 201 | Converted from Brinell Hardness |
| Hardness, Rockwell B | 88 | 88 | |
| Hardness, Vickers | 189 | 189 | Converted from Brinell Hardness. |
| Tensile Strength, Ultimate | 689 MPa | 99900 psi | |
| Tensile Strength, Yield | 345 MPa | 50000 psi | |
| Elongation at Break | 45 % | 45 % | in 50 mm |
| Modulus of Elasticity | 200 GPa | 29000 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 7.7e-005 ohm-cm | 7.7e-005 ohm-cm | at 20ºC |
| Magnetic Permeability | 1.02 | 1.02 | approximate value for the annealed condition at RT |
Thermal Properties |
|
| CTE, linear 250°C | 15.1 µm/m-°C | 8.39 µin/in-°F | at 0-315°C (32-600°F) |
| CTE, linear 500°C | 17.6 µm/m-°C | 9.78 µin/in-°F | 0 - 815ºC |
| Specific Heat Capacity | 0.5 J/g-°C | 0.12 BTU/lb-°F | from 0-100°C (32-212°F) |
| Thermal Conductivity at Elevated Temperature | 17.5 W/m-K | 121 BTU-in/hr-ft²-°F | 100ºC |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|