Titanium Ti-8Al-1Mo-1V (Ti-8-1-1), Beta Annealed, Aged
Subcategory: Alpha/Near Alpha Titanium Alloy; Metal; Nonferrous Metal; Titanium Alloy
Close Analogs: 5 other heat treatments of this alloy are in MatWeb.
Key Words: Ti8Al1Mo1V, UNS R54810; Ti-811
| Component | Wt. % |  | | | Al | 8 | | | Mo | 1 | | | Ti | 90 | | | V | 1 | |
|
Material Notes: Information provided by Allvac and the references. Annealed at 1065ºC, Aged at 595ºC. Applications: Fan & compressor blades, discs, spacers, seals, rings. Excellent creep resistance.
| Physical Properties | Metric | English | Comments |
|
| Density | 4.37 g/cc | 0.158 lb/in³ | |
Mechanical Properties |
|
| Tensile Strength, Ultimate | 1020 MPa | 148000 psi | |
| Tensile Strength, Yield | 900 MPa | 131000 psi | |
| Elongation at Break | 13 % | 13 % | |
| Modulus of Elasticity | 120 GPa | 17400 ksi | unspecified heat treatment |
| Poisson's Ratio | 0.32 | 0.32 | duplex annealed |
| Shear Modulus | 46 GPa | 6670 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 0.000197 ohm-cm | 0.000197 ohm-cm | |
Thermal Properties |
|
| CTE, linear 20°C | 8.5 µm/m-°C | 4.72 µin/in-°F | |
| CTE, linear 250°C | 9.2 µm/m-°C | 5.11 µin/in-°F | |
| CTE, linear 500°C | 10.1 µm/m-°C | 5.61 µin/in-°F | |
| Specific Heat Capacity | 0.502 J/g-°C | 0.12 BTU/lb-°F | |
| Thermal Conductivity | 6 W/m-K | 41.6 BTU-in/hr-ft²-°F | |
| Melting Point | Max 1540 °C | Max 2800 °F | Liquidus |
| Liquidus | 1540 °C | 2800 °F | |
| Beta Transus | 1040 °C | 1900 °F | |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|