Titanium Ti-8Al-1Mo-1V (Ti-8-1-1) Duplex Anneal
Subcategory: Alpha/Near Alpha Titanium Alloy; Metal; Nonferrous Metal; Titanium Alloy
Close Analogs: 5 other heat treatments of this alloy are in MatWeb.
Key Words: Ti8Al1Mo1V, DA, UNS R54810; Ti-811
| Component | Wt. % |  | | | Al | 8 | | | Mo | 1 | | | Ti | 90 | | | V | 1 | |
|
Material Notes: Information provided by Allvac and the references. Duplex Anneal: 980ºC 4h; air cool; 540ºC 24 h; air cool. Applications: Fan & compressor blades, discs, spacers, seals, rings. Excellent creep resistance.
| Physical Properties | Metric | English | Comments |
|
| Density | 4.37 g/cc | 0.158 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 326 | 326 | Estimated from Rockwell C. |
| Hardness, Knoop | 354 | 354 | Estimated from Rockwell C. |
| Hardness, Rockwell C | 35 | 35 | |
| Hardness, Vickers | 341 | 341 | Estimated from Rockwell C. |
| Tensile Strength, Ultimate | 900 - 1000 MPa | 131000 - 145000 psi | |
| Tensile Strength, Yield | 830 - 951 MPa | 120000 - 138000 psi | |
| Modulus of Elasticity | 124 GPa | 18000 ksi | |
| Poisson's Ratio | 0.32 | 0.32 | |
| Charpy Impact | 20 - 34 J | 14.8 - 25.1 ft-lb | V-notch |
| Fatigue Strength | 620 MPa | 89900 psi | 3,000,000 cycles, Unnotched |
| Fatigue Strength | 724 MPa | 105000 psi | at 85,000 Cycles |
| Fracture Toughness | 176 MPa-m½ | 160 ksi-in½ | K(IC) |
| Fracture Toughness | 374 MPa-m½ | 340 ksi-in½ | K(C) |
| Shear Modulus | 46 GPa | 6670 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 0.000198 ohm-cm | 0.000198 ohm-cm | |
Thermal Properties |
|
| CTE, linear 20°C | 8.5 µm/m-°C | 4.72 µin/in-°F | |
| CTE, linear 250°C | 9.2 µm/m-°C | 5.11 µin/in-°F | |
| CTE, linear 500°C | 10.1 µm/m-°C | 5.61 µin/in-°F | |
| Specific Heat Capacity | 0.502 J/g-°C | 0.12 BTU/lb-°F | |
| Thermal Conductivity | 6 W/m-K | 41.6 BTU-in/hr-ft²-°F | |
| Melting Point | Max 1540 °C | Max 2800 °F | Liquidus |
| Liquidus | 1540 °C | 2800 °F | |
| Beta Transus | 1038 °C | 1900 °F | |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your