Haynes® Waspaloy™ alloy, sheet, tested at 650°C (1200°F)
Subcategory: Metal; Nickel Base; Superalloy
Key Words: AMS 5544
| Component | Wt. % |  | | | Al | 1.5 | | | B | 0.006 | | | C | 0.08 | | | Co | 13.5 | |
| | Component | Wt. % |  | | | Cr | 19 | | | Fe | Max 2 | | | Mn | Max 0.1 | | | Mo | 4.3 | |
| | Component | Wt. % |  | | | Ni | 56 | | | Si | Max 0.15 | | | Ti | 3 | | | Zr | 0.05 | |
|
Material Notes: Nickel content to balance. Age-hardenable superalloy with very good strength at temperatures up 980°C (1800°F), can be cold-formed in the annealed condition, may also be hot formed at 1040°C (1900°F) and above, good resistance to gas turbine combustion gas environments at temperatures up to 870°C (1600°F). Widely used as a wrought material for forged and fabricated gas turbine and aerospace components. Data provided by the manufacturer, Haynes International, Inc.
| Physical Properties | Metric | English | Comments |
|
| Density | 8.2 g/cc | 0.296 lb/in³ | at RT |
Mechanical Properties |
|
| Tensile Strength, Ultimate | 1195 MPa | 173000 psi | |
| Tensile Strength, Yield | 770 MPa | 112000 psi | at 0.2% offset |
| Elongation at Break | 20.8 % | 20.8 % | in 51 mm |
| Modulus of Elasticity | 213 GPa | 30900 ksi | 20°C |
| Modulus of Elasticity at Elevated Temperature | 146 GPa | 21200 ksi | 1000°C (1830°F) |
| Modulus of Elasticity at Elevated Temperature | 155 GPa | 22500 ksi | 900°C (1650°F) |
| Modulus of Elasticity at Elevated Temperature | 164 GPa | 23800 ksi | 800°C (1470°F) |
| Modulus of Elasticity at Elevated Temperature | 172 GPa | 24900 ksi | 700°C (1290°F) |
| Modulus of Elasticity at Elevated Temperature | 180 GPa | 26100 ksi | 600°C (1110°F) |
| Modulus of Elasticity at Elevated Temperature | 192 GPa | 27800 ksi | 400°C (750°F) |
| Modulus of Elasticity at Elevated Temperature | 204 GPa | 29600 ksi | 200°C (390°F) |
Thermal Properties |
|
| CTE, linear 500°C | 13.9 µm/m-°C | 7.72 µin/in-°F | 20-500°C (68-930°F) |
| CTE, linear 1000°C | 14.3 µm/m-°C | 7.94 µin/in-°F | 20-600°C (68-1110°F) |
| CTE, linear 1000°C | 14.8 µm/m-°C | 8.22 µin/in-°F | 20-700°C (68-1290°F) |
| CTE, linear 1000°C | 15.4 µm/m-°C | 8.56 µin/in-°F | 20-800°C (68-1470°F) |
| CTE, linear 1000°C | 16.4 µm/m-°C | 9.11 µin/in-°F | 20-900°C (68-1650°F) |
| CTE, linear 1000°C | 17.8 µm/m-°C | 9.89 µin/in-°F | 20-1000°C (68-1830°F) |
| Thermal Conductivity at Elevated Temperature | 12.6 W/m-K | 87.4 BTU-in/hr-ft²-°F | 200°C (390°F) |
| Thermal Conductivity at Elevated Temperature | 15.7 W/m-K | 109 BTU-in/hr-ft²-°F | 400°C (750°F) |
| Thermal Conductivity at Elevated Temperature | 19.1 W/m-K | 133 BTU-in/hr-ft²-°F | 600°C (1110°F) |
| Thermal Conductivity at Elevated Temperature | 20.9 W/m-K | 145 BTU-in/hr-ft²-°F | 700°C (1290°F) |
| Thermal Conductivity at Elevated Temperature | 22.7 W/m-K | 158 BTU-in/hr-ft²-°F | 800°C (1470°F) |
| Thermal Conductivity at Elevated Temperature | 24.5 W/m-K | 170 BTU-in/hr-ft²-°F | 900°C (1650°F) |
| Melting Point | 1330 - 1360 °C | 2430 - 2480 °F | |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your