AISI 4130 Steel, normalized at 870°C (1600°F), air cooled, 25 mm (1 in.) round


Subcategory: AISI 4000 Series Steel; Ferrous Metal; Low Alloy Steel; Medium Carbon Steel; Metal

Key Words: alloy steels, UNS G41300, AMS 6350, AMS 6356, AMS 6360, AMS 6361, AMS 6372, AMS 6370, AMS 6371, AMS 6373, ASTM A322, ASTM A331, ASTM A505, ASTM A513, ASTM A519, ASTM A646, JIS SCM 2, JIS SCCrM 1, SS14 2225 (Sweden), B.S. CDS 110 (UK), medium carbon steels, chromium-molybdenum, chrome-moly, MIL SPEC MIL-S-16974, SAE J404, SAE J412, SAE J770, DIN 1.7218, AFNOR 25 CD 4 (France), MIL-S-6758 (flat and round bar), MIS-S-18729 ANN and NORM (sheet and plate), QQS-624 (round bar)

Component   Wt. %
C0.28 - 0.33 
Cr0.8 - 1.1 
Fe97.3 - 98.22 
Mn0.4 - 0.6 
Mo0.15 - 0.25 
PMax 0.035 
SMax 0.04 
Si0.15 - 0.35 

Material Notes:
Normalized: heated to 870°C, air cooled.

Physical PropertiesMetricEnglishComments
Density7.85 g/cc0.284 lb/in³ 

Mechanical Properties
Hardness, Brinell197197 
Hardness, Knoop219219 Converted from Brinell hardness.
Hardness, Rockwell B9292 Converted from Brinell hardness.
Hardness, Rockwell C1313 Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
Hardness, Vickers207207 Converted from Brinell hardness.
Tensile Strength, Ultimate670 MPa97200 psi 
Tensile Strength, Yield435 MPa63100 psi 
Elongation at Break25.5 %25.5 % in 50 mm
Reduction of Area59.5 %59.5 % 
Modulus of Elasticity205 GPa29700 ksi Typical for steel
Bulk Modulus140 GPa20300 ksi Typical for steel
Poisson's Ratio0.290.29 Calculated
Machinability70 %70 % annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus80 GPa11600 ksi Typical for steel

Electrical Properties
Electrical Resistivity2.23e-005 ohm-cm2.23e-005 ohm-cm specimen hardened and tempered; 20°C (68°F)
Electrical Resistivity at Elevated Temperature0.0001103 ohm-cm0.0001103 ohm-cm specimen hardened and tempered; 800°C (1470°F)
Electrical Resistivity at Elevated Temperature0.0001171 ohm-cm0.0001171 ohm-cm specimen hardened and tempered; 1000°C (1830°F)
Electrical Resistivity at Elevated Temperature0.0001222 ohm-cm0.0001222 ohm-cm specimen hardened and tempered; 1200°C (2192°F)
Electrical Resistivity at Elevated Temperature2.71e-005 ohm-cm2.71e-005 ohm-cm specimen hardened and tempered; 100°C (212°F)
Electrical Resistivity at Elevated Temperature3.42e-005 ohm-cm3.42e-005 ohm-cm specimen hardened and tempered; 200°C (390°F)
Electrical Resistivity at Elevated Temperature5.29e-005 ohm-cm5.29e-005 ohm-cm specimen hardened and tempered; 400°C (750°F)
Electrical Resistivity at Elevated Temperature7.86e-005 ohm-cm7.86e-005 ohm-cm specimen hardened and tempered; 600°C (1110°F)

Thermal Properties
Specific Heat Capacity0.477 J/g-°C0.114 BTU/lb-°F 50-100°C
Specific Heat Capacity at Elevated Temperature0.523 J/g-°C0.125 BTU/lb-°F 150-200°C
Specific Heat Capacity at Elevated Temperature0.837 J/g-°C0.2 BTU/lb-°F 750-800°C
Thermal Conductivity42.7 W/m-K296 BTU-in/hr-ft²-°F 100°C
Thermal Conductivity at Elevated Temperature30.1 W/m-K209 BTU-in/hr-ft²-°F 1200°C
Thermal Conductivity at Elevated Temperature40.7 W/m-K282 BTU-in/hr-ft²-°F 300°C

References for this datasheet.


Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistant format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. MatWeb data and tools provided by MatWeb, LLC.