AISI 8620 Steel, direct quenched from pot, 150°C (300°F) temper, carburized
Subcategory: AISI 8000 Series Steel; Ferrous Metal; Low Alloy Steel; Low Carbon Steel; Metal
Close Analogs: AISI 8620H
Key Words: AFNOR 22 NCD 2, UNI 20 NiCrMo 2, JIS SNCM 21 H, JIS SNCM 21, B.S. 805 H 20 (UK), B.S. 805 M 20 (UK), MIL SPEC MIL-S-16794, SAE J404, SAE J770, DIN 1.6523, AFNOR 20 NCD 2 (France), UNS G86200, AMS 6274, AMS 6276, AMS 6277, ASTM A322, ASTM A331, ASTM A505, ASTM A526
| Component | Wt. % |  | | | C | 0.18 - 0.23 | | | Cr | 0.4 - 0.6 | | | Fe | 96.9 - 98.02 | |
| | Component | Wt. % |  | | | Mn | 0.7 - 0.9 | | | Mo | 0.15 - 0.25 | | | Ni | 0.4 - 0.7 | |
| | Component | Wt. % |  | | | P | Max 0.035 | | | S | Max 0.04 | | | Si | 0.15 - 0.35 | |
|
Material Notes: Direct quenched from pot: carburized at 925°C (1700°F) for 8 hrs., quenched in agitated oil, 150°C (300°F) temper. Core properties.
| Physical Properties | Metric | English | Comments |
|
| Density | 7.85 g/cc | 0.284 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 388 | 388 | |
| Hardness, Knoop | 418 | 418 | Converted from Brinell hardness. |
| Hardness, Rockwell B | 101 | 101 | Converted from Brinell hardness. |
| Hardness, Rockwell C | 63 | 63 | case hardness. |
| Hardness, Vickers | 411 | 411 | Converted from Brinell hardness. |
| Tensile Strength, Ultimate | 1324 MPa | 192000 psi | |
| Tensile Strength, Yield | 1036 MPa | 150000 psi | |
| Elongation at Break | 12.5 % | 12.5 % | in 50 mm. |
| Reduction of Area | 49.4 % | 49.4 % | |
| Modulus of Elasticity | 205 GPa | 29700 ksi | Typical for steel |
| Bulk Modulus | 140 GPa | 20300 ksi | Typical for steels |
| Poisson's Ratio | 0.29 | 0.29 | Calculated |
| Machinability | 65 % | 65 % | hot rolled and cold drawn. Based on 100% machinability for AISI 1212 steel. |
| Shear Modulus | 80 GPa | 11600 ksi | Typical for steel. |
Electrical Properties |
|
| Electrical Resistivity | 2.34e-005 ohm-cm | 2.34e-005 ohm-cm | Typical steel |
Thermal Properties |
|
| Specific Heat Capacity | 0.475 J/g-°C | 0.114 BTU/lb-°F | Typical steel |
| Thermal Conductivity | 46.6 W/m-K | 323 BTU-in/hr-ft²-°F | Typical steel |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use