| Aluminum 7475-T761
 Subcategory: 7000 Series Aluminum Alloy; Aluminum Alloy; Metal; Nonferrous Metal Close Analogs:  Composition Notes: Aluminum content reported is calculated as remainder.
 Composition information provided by the Aluminum Association and is not for design.
 Key Words: UNS A97475; ISO AlZn5.5MgCu(A); Aluminium 7475-T761; AA7475-T761 | | Component | Wt. % |  |  |  |  | Al | 88.5 - 91.5 |  |  | Cr | 0.18 - 0.25 |  |  | Cu | 1.2 - 1.9 |  |  | Fe | Max 0.12 |  | 
 | | Component | Wt. % |  |  |  |  | Mg | 1.9 - 2.6 |  |  | Mn | Max 0.06 |  |  | Other, each | Max 0.05 |  |  | Other, total | Max 0.15 |  | 
 | | Component | Wt. % |  |  |  |  | Si | Max 0.1 |  |  | Ti | Max 0.06 |  |  | Zn | 5.2 - 6.2 |  | 
 | 
 Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.
 
| Physical Properties | Metric | English | Comments |  |  |  | Density | 2.81 g/cc | 0.102 lb/in³ | AA; Typical |  | Mechanical Properties
 |  |  |  | Hardness, Brinell | 140 | 140 | 500 kg load with 10 mm ball.  Calculated value. |  | Hardness, Knoop | 177 | 177 | Converted from Brinell Hardness Value |  | Hardness, Rockwell A | 51.6 | 51.6 | Converted from Brinell Hardness Value |  | Hardness, Rockwell B | 84 | 84 | Converted from Brinell Hardness Value |  | Hardness, Vickers | 162 | 162 | Converted from Brinell Hardness Value |  | Ultimate Tensile Strength | 517 MPa | 75000 psi | AA; Typical |  | Tensile Yield Strength | 448 MPa | 65000 psi | AA; Typical |  | Elongation at Break | 12 % | 12 % | AA; Typical; 1/16 in. (1.6 mm) Thickness |  | Modulus of Elasticity | 70.3 GPa | 10200 ksi | AA; Typical; Average of tension and compression.  Compression modulus is about 2% greater than tensile modulus. |  | Poisson's Ratio | 0.33 | 0.33 |  |  | Shear Modulus | 27 GPa | 3920 ksi |  |  | Shear Strength | 310 MPa | 45000 psi | Calculated value. |  | Electrical Properties
 |  |  |  | Electrical Resistivity | 4.32e-006 ohm-cm | 4.32e-006 ohm-cm | AA; Typical at 68°F |  | Thermal Properties
 |  |  |  | CTE, linear 68°F | 23.2 µm/m-°C | 12.9 µin/in-°F | AA; Typical; Average over 68-212°F range. |  | CTE, linear 250°C | 25.2 µm/m-°C | 14 µin/in-°F | Average over the range 20-300ºC |  | Specific Heat Capacity | 0.88 J/g-°C | 0.21 BTU/lb-°F | Estimated from trends in similar Al alloys. |  | Thermal Conductivity | 147 W/m-K | 1020 BTU-in/hr-ft²-°F | AA; Typical at 77°F |  | Melting Point | 477 - 635 °C | 890 - 1175 °F | AA; Typical range based on typical composition for wrought products 1/4 inch thickness or greater |  | Solidus | 477 °C | 890 °F | AA; Typical |  | Liquidus | 635 °C | 1175 °F | AA; Typical |  | Processing Properties
 |  |  |  | Annealing Temperature | 413 °C | 775 °F |  |  | Solution Temperature | 516 °C | 960 °F | must be preceded by soak at 870 to 890°F |  | Aging Temperature | 121 - 177 °C | 250 - 350 °F |  |  References for this datasheet. Some of the values displayed above may have been converted from their original units and/or rounded in 
	order to display the information in a consistant format.  Users requiring more precise data for scientific or 
	engineering calculations can click on the property value to see the original value as well as raw conversions 
	to equivalent units.  We advise that you only use the original value or one of its raw conversions in your 
	calculations to minimize rounding error.  We also ask that you refer to MatWeb's disclaimer and terms of use 
	regarding this information.  MatWeb data and tools provided by MatWeb, LLC.
 
 |