AISI Type 303 Stainless Steel, annealed bar, tested at RT
Subcategory: Ferrous Metal; Heat Resisting; Metal; Stainless Steel; T 300 Series Stainless Steel
Close Analogs: AISI Type 303 Se
Key Words: T303, T 303, 303SS, 303 SS, AFNOR Z 10 CNF 18.09 (Fr), UNI X 10 CrNiS 18 09, SUS 303, SS14 2346 (Sweden), B.S. 303 S 21, UNS S30300, AMS 5640 (1), ASME SA194, ASME SA320, ASTM A194, ASTM A314, ASTM A320, ASTM A320, ASTM A473, ASTM A581, ASTM A582, MIL SPEC MIL-S-862, SAE J405 (30303), DIN 1.4305, X12CrNiS188, EN 58M, austenitic, ISO 683/13 17, 18-8
| Component | Wt. % |  | | | C | Max 0.15 | | | Cr | 18 | | | Fe | 69 | |
| | Component | Wt. % |  | | | Mn | Max 2 | | | Mo | Max 0.6 | | | Ni | 9 | |
| | Component | Wt. % |  | | | P | Max 0.2 | | | S | Min 0.15 | | | Si | Max 1 | |
|
| Physical Properties | Metric | English | Comments |
|
| Density | 8 g/cc | 0.289 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 160 | 160 | |
| Hardness, Knoop | 180 | 180 | Converted from Brinell hardness. |
| Hardness, Rockwell B | 83 | 83 | Converted from Brinell hardness. |
| Hardness, Vickers | 167 | 167 | Converted from Brinell hardness. |
| Tensile Strength, Ultimate | 620 MPa | 89900 psi | |
| Tensile Strength, Yield | 240 MPa | 34800 psi | at 0.2% offset |
| Elongation at Break | 50 % | 50 % | in 50 mm |
| Modulus of Elasticity | 193 GPa | 28000 ksi | tension |
| Poisson's Ratio | 0.25 | 0.25 | Calculated |
| Fatigue Strength | 240 MPa | 34800 psi | annealed |
| Fatigue Strength | 330 MPa | 47900 psi | 25% hardened |
| Shear Modulus | 77.2 GPa | 11200 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 7.2e-005 ohm-cm | 7.2e-005 ohm-cm | |
| Magnetic Permeability | 1.008 | 1.008 | at RT |
Thermal Properties |
|
| CTE, linear 20°C | 17.2 µm/m-°C | 9.56 µin/in-°F | from from 0-100°C |
| CTE, linear 250°C | 17.8 µm/m-°C | 9.89 µin/in-°F | at 0-315°C (32-600°F) |
| CTE, linear 500°C | 18.4 µm/m-°C | 10.2 µin/in-°F | at 0-540°C, 18.7 µm/m-C at 0-650°C |
| Specific Heat Capacity | 0.5 J/g-°C | 0.12 BTU/lb-°F | from 0-100°C (32-212°F) |
| Thermal Conductivity | 16.2 W/m-K | 112 BTU-in/hr-ft²-°F | at 100°C (212°F), 21.5 W/m-K at 500°C (930°F) |
| Melting Point | 1400 - 1420 °C | 2550 - 2590 °F | |
| Solidus | 1400 °C | 2550 °F | |
| Liquidus | 1420 °C | 2590 °F | |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|