AISI Type 303 Se Stainless Steel, cold drawn, bar, tested at RT
 Subcategory: Ferrous Metal; Heat Resisting; Metal; Stainless Steel; T 300 Series Stainless Steel 
Close Analogs: AISI Type 303 
Key Words: T303, T 303, 303Se, 303SS, 303 SS, UNS S30323, AMS 5640 (type 2), AMS 5641, AMS 5738, ASME SA194, ASME SA320, ASTM A194, ASTM A194 (8F), ASTM A314, ASTM A320, ASTM A473, ASTM A581, ASTM A582, MIL SPEC MIL-S-862, SAE J405 (30303 Se), DIN 1.4305, X12CrNiS188, B.S. 303 S 41, EN 58M, , austenitic, 18-8 
| Component |    Wt. % |   |   |  | C | Max 0.15 |   |  | Cr | 18 |   |  | Fe | 69 |   |  
  | | Component |    Wt. % |   |   |  | Mn | Max 2 |   |  | Ni | 9 |   |  | P | Max 0.2 |   |  
  | | Component |    Wt. % |   |   |  | S | Max 0.06 |   |  | Se | Max 0.15 |   |  | Si | Max 1 |   |  
  |   
| Physical Properties | Metric | English | Comments |  
 |  
| Density | 8 g/cc | 0.289 lb/in³ |   |  
 Mechanical Properties |  
 |  
| Hardness, Brinell | 228 | 228 |   |  
| Hardness, Knoop | 251 | 251 |  Converted from Brinell hardness. |  
| Hardness, Rockwell B | 96 | 96 |  Converted from Brinell hardness. |  
| Hardness, Rockwell C | 19 | 19 |  Converted from Brinell hardness. Value below normal HRC range, for comparison only. |  
| Hardness, Vickers | 240 | 240 |  Converted from Brinell hardness. |  
| Tensile Strength, Ultimate | 690 MPa | 100000 psi |   |  
| Tensile Strength, Yield | 415 MPa | 60200 psi |  at 0.2% offset |  
| Elongation at Break | 40 % | 40 % |  in 50 mm |  
| Modulus of Elasticity | 193 GPa | 28000 ksi |  tension |  
| Poisson's Ratio | 0.25 | 0.25 |  Calculated |  
| Shear Modulus | 77.2 GPa | 11200 ksi |   |  
 Electrical Properties |  
 |  
| Electrical Resistivity | 7.2e-005 ohm-cm | 7.2e-005 ohm-cm |   |  
 Thermal Properties |  
 |  
| CTE, linear 20°C | 17.2 µm/m-°C | 9.56 µin/in-°F |  from from 0-100°C |  
| CTE, linear 250°C | 17.8 µm/m-°C | 9.89 µin/in-°F |  at 0-315°C (32-600°F) |  
| CTE, linear 500°C | 18.4 µm/m-°C | 10.2 µin/in-°F |  at 0-540°C, 18.7 µm/m-C at 0-650°C |  
| Specific Heat Capacity | 0.5 J/g-°C | 0.12 BTU/lb-°F |  from 0-100°C (32-212°F) |  
| Thermal Conductivity | 16.2 W/m-K | 112 BTU-in/hr-ft²-°F |  at 100°C (212°F), 21.5 W/m-K at 500°C (930°F) |  
| Melting Point | 1400 - 1420 °C | 2550 - 2590 °F |   |  
| Solidus | 1400 °C | 2550 °F |   |  
| Liquidus | 1420 °C | 2590 °F |   |  
 
References for this datasheet. 
	 Some of the values displayed above may have been converted from their original units and/or rounded in 
	order to display the information in a consistant format.  Users requiring more precise data for scientific or 
	engineering calculations can click on the property value to see the original value as well as raw conversions 
	to equivalent units.  We advise that you only use the original value or one of its raw conversions in your 
	calculations to minimize rounding error.  We also ask that you refer to MatWeb's disclaimer and terms of use 
	regarding this information.  MatWeb data and tools provided by MatWeb, LLC. 
				 |