AISI Type 316 Stainless Steel, annealed plate
Subcategory: Ferrous Metal; Metal; Stainless Steel; T 300 Series Stainless Steel
Key Words: UNS S31600, SS316, 316SS, AISI 316, DIN 1.4401, DIN 1.4408, DIN X5CrNiMo17122, TGL 39672 X5CrNiMo1911, TGL 7143X5CrNiMo1811, ISO 2604-1 F62, ISO 2604-2 TS60, ISO 2604-2 TS61, ISO 2604-4 P60, ISO 2604-4 P61, ISO 4954 X5CrNiMo17122E, ISO 683/13 20, ISO 683/13 20a, ISO 6931 X5CrNiMo17122, JIS SUS 316
| Component | Wt. % |  | | | C | 0.08 | | | Cr | 17 | | | Fe | 65 | |
| | Component | Wt. % |  | | | Mn | 2 | | | Mo | 2.5 | | | Ni | 12 | |
| | Component | Wt. % |  | | | P | 0.045 | | | S | 0.03 | | | Si | 1 | |
|
Material Notes: Molybdenum content increases resistance to marine environments. High creep strength at elevated temperatures and good heat resistance. Biocompatible. Fabrication characteristics similar to Types 302 and 304. Applications: food and pharmaceutical processing equipment, marine exterior trim, surgical implants, and industrial equipment that handles the corrosive process chemicals used to produce inks, rayons, photographic chemicals, paper, textiles, bleaches, and rubber. Corrosion Resistance: better corrosion resistance than 302 and 304; resists sodium and calcium brines; hypochlorite solutions, phosphoric acid; and the sulfite liquors and sulfurous acids used in the paper pulp industry.
| Physical Properties | Metric | English | Comments |
|
| Density | 8 g/cc | 0.289 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 149 | 149 | |
| Hardness, Knoop | 169 | 169 | Converted from Brinell hardness. |
| Hardness, Rockwell B | 80 | 80 | |
| Hardness, Vickers | 155 | 155 | Converted from Brinell hardness. |
| Tensile Strength, Ultimate | 565 MPa | 81900 psi | |
| Tensile Strength, Yield | 250 MPa | 36300 psi | |
| Elongation at Break | 55 % | 55 % | in 50 mm |
| Modulus of Elasticity | 193 GPa | 28000 ksi | |
| Charpy Impact | 105 J | 77.4 ft-lb | V-notch |
| Izod Impact | 129 J | 95.1 ft-lb | |
Electrical Properties |
|
| Electrical Resistivity | 7.4e-005 ohm-cm | 7.4e-005 ohm-cm | at 20ºC |
| Magnetic Permeability | 1.008 | 1.008 | at RT |
Thermal Properties |
|
| CTE, linear 20°C | 16 µm/m-°C | 8.89 µin/in-°F | 0 - 100ºC |
| CTE, linear 250°C | 16.2 µm/m-°C | 9 µin/in-°F | at 0-315°C (32-600°F) |
| CTE, linear 500°C | 17.5 µm/m-°C | 9.72 µin/in-°F | 0 - 540ºC |
| Specific Heat Capacity | 0.5 J/g-°C | 0.12 BTU/lb-°F | from 0-100°C (32-212°F) |
| Thermal Conductivity at Elevated Temperature | 16.3 W/m-K | 113 BTU-in/hr-ft²-°F | 100ºC |
| Melting Point | 1370 - 1400 °C | 2500 - 2550 °F | |
| Solidus | 1370 °C | 2500 °F | |
| Liquidus | 1400 °C | 2550 °F | |
| Maximum Service Temperature, Air | 870 °C | 1600 °F | Intermittent Service |
| Maximum Service Temperature, Air | 925 °C | 1700 °F | Continuous Service |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|