AISI Type 316L Stainless Steel, annealed sheet
Subcategory: Ferrous Metal; Metal; Stainless Steel; T 300 Series Stainless Steel
Key Words: UNS S31603, AISI 316L, ISO 2604-1 F59, ISO 2604-4 P57, ISO 2604-4 P58, ISO 4954 X2CrNiMo17133E, ISO 683/13 19, ISO 683/13 19a, biomaterials, biomedical implants, biocompatible materials
| Component | Wt. % |  | | | C | 0.03 | | | Cr | 17 | | | Fe | 65 | |
| | Component | Wt. % |  | | | Mn | 2 | | | Mo | 2.5 | | | Ni | 12 | |
| | Component | Wt. % |  | | | P | 0.045 | | | S | 0.03 | | | Si | 1 | |
|
Material Notes: Similar to Type 316 for superior corrosion resistance, but also has superior resistance to intergranular corrosion following welding or stress relieving. Good corrosion resistance to most chemicals, salts, and acids and molybdenum content helps resistance to marine environments. The low carbon content of 316L reduces the possibility of in vivo corrosion for medical implant use. High creep strength at elevated temperatures. 316L has fabrication characteristics similar to Types 302 and 304. Applications: biomedical implants, chemical processing, food processing, photographic, pharmaceutical, textile finishing, marine exterior trim.
| Physical Properties | Metric | English | Comments |
|
| Density | 8 g/cc | 0.289 lb/in³ | |
Mechanical Properties |
|
| Hardness, Rockwell B | 79 | 79 | |
| Tensile Strength, Ultimate | 560 MPa | 81200 psi | |
| Tensile Strength, Yield | 290 MPa | 42100 psi | |
| Elongation at Break | 50 % | 50 % | in 50 mm |
| Modulus of Elasticity | 193 GPa | 28000 ksi | in tension |
| Charpy Impact | 103 J | 76 ft-lb | V-notch, 30ºC |
| Izod Impact | 150 J | 111 ft-lb | 21ºC, 150 J at -195°C(-320°F) |
Electrical Properties |
|
| Electrical Resistivity | 7.4e-005 ohm-cm | 7.4e-005 ohm-cm | at 20ºC |
| Magnetic Permeability | 1.008 | 1.008 | at RT |
Thermal Properties |
|
| Specific Heat Capacity | 0.5 J/g-°C | 0.12 BTU/lb-°F | from 0-100°C (32-212°F) |
| Melting Point | 1375 - 1400 °C | 2510 - 2550 °F | |
| Solidus | 1375 °C | 2510 °F | |
| Liquidus | 1400 °C | 2550 °F | |
| Maximum Service Temperature, Air | 870 °C | 1600 °F | Intermittent Service |
| Maximum Service Temperature, Air | 925 °C | 1700 °F | Continuous Service |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|