AISI Type S15500 (15Cr-5Ni) Precipitation Hardening Stainless Steel tested at 24°C (75.2°F), condition H925
Subcategory: Ferrous Metal; Metal; Precipitation Hardening Stainless; Stainless Steel; T S10000 Series Stainless Steel
Key Words: 15-5 PH, 15-5PH, 15/5 PH, 15/5PH, XM12, AMS 5862, ASME SA705 (XM-12), ASTM A564 (XM-12), ASTM A693 (XM-12), ASTM A705 (XM-12), AFNOR NF A35-581 Z6CNU15.05, DIN 1.4540, DIN X4CrNiCuNb164, Cr-Ni 15-5, UNS S15500, AMS 5658, AMS 5659, AMS 5826
| Component | Wt. % |  | | | C | Max 0.07 | | | Cr | 14.8 | | | Cu | 3.5 | | | Fe | 75 | |
| | Component | Wt. % |  | | | Mn | Max 1 | | | Nb + Ta | 0.3 | | | Ni | 4.5 | |
| | Component | Wt. % |  | | | P | Max 0.04 | | | S | Max 0.03 | | | Si | Max 1 | |
|
Material Notes: Martensitic, precipitative hardening (maraging), combining high strength and hardness with excellent corrosion resistance. Applications include valve parts, fittings and fasteners, shafts, gears, chemical process equipment, paper mill equipment, aircraft components and nuclear reactor components.
| Physical Properties | Metric | English | Comments |
|
| Density | 7.8 g/cc | 0.282 lb/in³ | |
Mechanical Properties |
|
| Tensile Strength, Ultimate | 1317 MPa | 191000 psi | |
| Tensile Strength, Yield | 1213 MPa | 176000 psi | |
| Elongation at Break | 16 % | 16 % | gage length is 4 times diameter |
| Charpy Impact | 79 J | 58.3 ft-lb | at 24°C, 38 J at -12°C, 22 J at -40°C, 9 J at -73°C |
Electrical Properties |
|
| Magnetic Permeability | 95 | 95 | approximate value for the annealed condition at RT |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|