17-7 PH Stainless Steel, CH900, plate, sheet, and strip
Subcategory: Ferrous Metal; Metal; Precipitation Hardening Stainless; Stainless Steel; T S10000 Series Stainless Steel
Key Words: UNS S17700, double treatment alloy, CH900, plate, sheet, and strip, 17-7PH, 17-7 PH, 17/7PH, 17/7 PH, Precipitation Hardening
| Component | Wt. % |  | | | Al | 0.75 - 1.5 | | | C | Max 0.09 | | | Cr | 16 - 18 | | | Mn | Max 1 | | | Ni | 6.5 - 7.75 | | | P | Max 0.04 | | | S | Max 0.04 | | | Si | Max 1 | |
|
Material Notes: Processing: CH900 - heated to austenitic range, 1040°C (1900°F), and water quenched. Severely cold worked (60-70%). The cold working induces a martensite transformation in the austenite. Tempered at 480°C (900°) Applications: high strength high temperature applications, chemical processing equipment, heat exchangers, power boilers, superheater tubes Corrosion Resistance: 17-7 PH is suitable for use in fresh water, industrial and marine atmospheres, and mild chemical and oxidizing environments. 17-7 PH should not be used in salt water or reducing environments.
| Physical Properties | Metric | English | Comments |
|
| Density | 7.8 g/cc | 0.282 lb/in³ | |
Mechanical Properties |
|
| Hardness, Rockwell C | 46 | 46 | |
| Tensile Strength, Ultimate | 1650 MPa | 239000 psi | |
| Tensile Strength, Yield | 1590 MPa | 231000 psi | |
| Elongation at Break | 1 % | 1 % | |
| Modulus of Elasticity | 204 GPa | 29600 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 8.3e-005 ohm-cm | 8.3e-005 ohm-cm | |
Thermal Properties |
|
| CTE, linear 20°C | 11 µm/m-°C | 6.11 µin/in-°F | from 0-100°C (32-212°F) |
| CTE, linear 250°C | 11.6 µm/m-°C | 6.44 µin/in-°F | from 0-315°C (32-600°F) |
| Specific Heat Capacity | 0.46 J/g-°C | 0.11 BTU/lb-°F | from 0-100°C (32-212°F) |
| Thermal Conductivity | 16.4 W/m-K | 114 BTU-in/hr-ft²-°F | at 100°C(212°F); 21.8 W/m-K at 500°C (930°F) |
| Melting Point | 1400 - 1450 °C | 2550 - 2640 °F | |
| Solidus | 1400 °C | 2550 °F | |
| Liquidus | 1450 °C | 2640 °F | |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|