17-7 PH Stainless Steel, TH1050, bar and forgings
Subcategory: Ferrous Metal; Metal; Precipitation Hardening Stainless; Stainless Steel; T S10000 Series Stainless Steel
Key Words: UNS S17700, double treatment alloy, TH1050, bar and forgings, 17-7PH, 17-7 PH, 17/7PH, 17/7 PH, Precipitation Hardening
| Component | Wt. % |  | | | Al | 0.75 - 1.5 | | | C | Max 0.09 | | | Cr | 16 - 18 | | | Mn | Max 1 | | | Ni | 6.5 - 7.75 | | | P | Max 0.04 | | | S | Max 0.04 | | | Si | Max 1 | |
|
Material Notes: Properties are measured in the longitudinal direction. Processing: TH1050 - heated to austenitic range, 1040°C (1900°F), and water quenched. Reheated to 760°C (1400°F) to precipitate carbides. Carbides cause the austenite transform to martensite after cooling below 15°C (60°F). Tempered at 565°C (1050°) Applications: high strength high temperature applications, chemical processing equipment, heat exchangers, power boilers, superheater tubes Corrosion Resistance: 17-7 PH is suitable for use in fresh water, industrial and marine atmospheres, and mild chemical and oxidizing environments. 17-7 PH should not be used in salt water or reducing environments.
| Physical Properties | Metric | English | Comments |
|
| Density | 7.8 g/cc | 0.282 lb/in³ | |
Mechanical Properties |
|
| Hardness, Rockwell C | 38 | 38 | |
| Tensile Strength, Ultimate | 1170 MPa | 170000 psi | |
| Tensile Strength, Yield | 965 MPa | 140000 psi | |
| Elongation at Break | 6 % | 6 % | |
| Reduction of Area | 25 % | 25 % | |
| Modulus of Elasticity | 204 GPa | 29600 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 8.3e-005 ohm-cm | 8.3e-005 ohm-cm | |
Thermal Properties |
|
| CTE, linear 20°C | 11 µm/m-°C | 6.11 µin/in-°F | from 0-100°C (32-212°F) |
| CTE, linear 250°C | 11.6 µm/m-°C | 6.44 µin/in-°F | from 0-315°C (32-600°F) |
| Specific Heat Capacity | 0.46 J/g-°C | 0.11 BTU/lb-°F | from 0-100°C (32-212°F) |
| Thermal Conductivity | 16.4 W/m-K | 114 BTU-in/hr-ft²-°F | at 100°C(212°F); 21.8 W/m-K at 500°C (930°F) |
| Melting Point | 1400 - 1450 °C | 2550 - 2640 °F | |
| Solidus | 1400 °C | 2550 °F | |
| Liquidus | 1450 °C | 2640 °F | |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|