AISI Type S21904 (Alloy 21-6-9) Stainless Steel, 30% final cold reduction, stress relieving heat treatment 620°C (1150°F) for 2 hours, air cooled
Subcategory: Ferrous Metal; Heat Resisting; Metal; Stainless Steel; T S20000 Series Stainless Steel
Close Analogs: AISI Type S21900
Key Words: UNS S21904, AMS 5595, AMS 5656, ASME SA412, ASTM A269 (XM-11), ASTM A276 (XM-11), ASTM A314 (XM-11), ASTM A412 (XM-11), ASTM A473 (XM-11), ASTM A580 (XM-11)
| Component | Wt. % |  | | | C | Max 0.04 | | | Cr | 20 | | | Fe | 64 | |
| | Component | Wt. % |  | | | Mn | 9 | | | N | 0.23 | | | Ni | 6 | |
| | Component | Wt. % |  | | | P | Max 0.06 | | | S | Max 0.03 | | | Si | Max 1 | |
|
Material Notes: Austenitic, high strength, excellent corrosion resistance, and low magnetic permeability. Applications include aircraft applications such as ducting and bellows systems, tail pipes and exhaust systems, clamps, fasteners, flanges, and hydraulic tubing.
| Physical Properties | Metric | English | Comments |
|
| Density | 7.83 g/cc | 0.283 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 311 | 311 | Converted from Rockwell C hardness. |
| Hardness, Knoop | 335 | 335 | Converted from Rockwell C hardness. |
| Hardness, Rockwell C | 33 | 33 | |
| Hardness, Vickers | 323 | 323 | Converted from Rockwell C hardness. |
| Tensile Strength, Ultimate | 1145 MPa | 166000 psi | |
| Tensile Strength, Yield | 1025 MPa | 149000 psi | at 0.2% offset |
| Elongation at Break | 28 % | 28 % | in 50 mm |
| Modulus of Elasticity | 200 GPa | 29000 ksi | Typical for stainless steel |
| Machinability | 30 % | 30 % | Based on 100% machinability for AISI 1212 steel. |
Electrical Properties |
|
| Electrical Resistivity | 7.3e-005 ohm-cm | 7.3e-005 ohm-cm | |
Thermal Properties |
|
| CTE, linear 20°C | 16.7 µm/m-°C | 9.28 µin/in-°F | at 25-95°C, 17.3 µm/m°C at 25-205°C. Annealed |
| CTE, linear 250°C | 18.2 µm/m-°C | 10.1 µin/in-°F | at 25-315°C. Annealed |
| CTE, linear 500°C | 19.1 µm/m-°C | 10.6 µin/in-°F | at 25-540°C, 20.0 µm/m-°C at 25-760°C, 20.0 µm/m-°C at 25-870°C, 20.5 µm/m-°C at 25-980°C. Annealed |
| Specific Heat Capacity | 0.48 J/g-°C | 0.115 BTU/lb-°F | Typical value for stainless steel. |
| Thermal Conductivity | 13.8 W/m-K | 95.8 BTU-in/hr-ft²-°F | 13.8 at 95°C, 7.8 W/m°C at -180°C, 10.9 W/m°C at -73°C, 16.1 W/m°C at 205°C, 18.2 W/m°C at 315°C, 20.2 W/m°C at 425°C, 22.5 W/m°C at 540°C, 24.7 W/m°C at 650°C, 26.8 W/m°C at 760°C, 28.9 W/m°C at 870°C |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|