Titanium Ti-15V-3Cr-3Al-3Sn Solution Treated
Subcategory: Beta Titanium Alloy; Metal; Nonferrous Metal; Titanium Alloy
Close Analogs: 3 other heat treatments of this alloy are in MatWeb.
Key Words: Titanium Ti-15-3
| Component | Wt. % |  | | | Al | 3 | | | Cr | 3 | | | Sn | 3 | | | Ti | 76 | | | V | 15 | |
|
| Physical Properties | Metric | English | Comments |
|
| Density | 4.76 g/cc | 0.172 lb/in³ | |
Mechanical Properties |
|
| Hardness, Rockwell B | 95 | 95 | |
| Tensile Strength, Ultimate | 790 MPa | 115000 psi | |
| Tensile Strength, Yield | 770 MPa | 112000 psi | |
| Elongation at Break | 22 % | 22 % | |
| Modulus of Elasticity | 82 GPa | 11900 ksi | |
| Poisson's Ratio | 0.33 | 0.33 | Typical for beta titanium alloy. |
| Shear Modulus | 30.8 GPa | 4470 ksi | Calculated from typical values. |
Electrical Properties |
|
| Electrical Resistivity | 0.00014 ohm-cm | 0.00014 ohm-cm | |
Thermal Properties |
|
| CTE, linear 20°C | 8.5 µm/m-°C | 4.72 µin/in-°F | 20-95ºC |
| CTE, linear 250°C | 9.1 µm/m-°C | 5.06 µin/in-°F | |
| CTE, linear 500°C | 9.8 µm/m-°C | 5.44 µin/in-°F | |
| Specific Heat Capacity | 0.5 J/g-°C | 0.12 BTU/lb-°F | at 20ºC. Value at 400ºC is 0.649 J/g-ºC |
| Thermal Conductivity | 8.08 W/m-K | 56.1 BTU-in/hr-ft²-°F | |
| Beta Transus | 760 °C | 1400 °F | |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|