Titanium Grade 3, Annealed
Subcategory: Metal; Nonferrous Metal; Titanium Alloy; Unalloyed/Modified Titanium
Close Analogs: Titanium Grades 1,2,3,4,7,11,and 12 are all considered unalloyed and have similar mechanical properties.
Key Words: ASTM Grade 3; UNS R50550, CP titanium, C.P. titanium alloy
| Component | Wt. % |  | | | C | Max 0.1 | | | Fe | Max 0.3 | | | H | Max 0.015 | | | N | Max 0.05 | | | O | Max 0.35 | | | Ti | 99.1 | |
|
Material Notes: Information provided by Allvac and the references. Applications: Airframe skin, heat exchangers, cryogenic vessels, components for CPI equipment, condenser tubing, exhaust pipe shrouds. Sample was annealed 2 hr at 700°C.
| Physical Properties | Metric | English | Comments |
|
| Density | 4.5 g/cc | 0.163 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 266 | 266 | Estimated from Rockwell C. |
| Hardness, Knoop | 289 | 289 | Estimated from Rockwell C. |
| Hardness, Rockwell C | 26 | 26 | |
| Hardness, Vickers | 280 | 280 | Estimated from Rockwell C. |
| Tensile Strength, Ultimate | 520 MPa | 75400 psi | |
| Tensile Strength, Yield | 450 MPa | 65300 psi | |
| Elongation at Break | 25 % | 25 % | |
| Modulus of Elasticity | 104 GPa | 15100 ksi | in tension. |
| Notched Tensile Strength | 790 MPa | 115000 psi | Kt (stress concentration factor) = 3.0 |
| Ultimate Bearing Strength | 920 MPa | 133000 psi | |
| Bearing Yield Strength | 650 MPa | 94300 psi | |
| Poisson's Ratio | 0.34 | 0.34 | |
| Charpy Impact | 27 J | 19.9 ft-lb | V-notch |
| Fatigue Strength | 250 MPa | 36300 psi | at 1E+7 cycles. Kt (stress concentration factor) = 2.7 |
| Fatigue Strength | 340 MPa | 49300 psi | 1E+7 cycles, Unnotched |
| Shear Modulus | 39 GPa | 5660 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 5.4e-005 ohm-cm | 5.4e-005 ohm-cm | |
Thermal Properties |
|
| Heat of Fusion | 325 J/g | 140 BTU/lb | High Purity Ti. |
| CTE, linear 20°C | 8.6 µm/m-°C | 4.78 µin/in-°F | 20-93°C |
| CTE, linear 250°C | 9.2 µm/m-°C | 5.11 µin/in-°F | Unspecified heat treatment. Average over the range 0-315ºC |
| Specific Heat Capacity | 0.523 J/g-°C | 0.125 BTU/lb-°F | |
| Thermal Conductivity | 16.4 W/m-K | 114 BTU-in/hr-ft²-°F | |
| Melting Point | Max 1660 °C | Max 3020 °F | Liquidus |
| Liquidus | 1660 °C | 3020 °F | |
| Beta Transus | 920 °C | 1690 °F | |
Optical Properties |
|
| Emissivity (0-1) | 0.3 | 0.3 | High purity Ti at 710°C |
| Reflection Coefficient, Visible (0-1) | 0.56 | 0.56 | High purity Ti; visible light. |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|