Vasco® 17-4 Precipitation Hardening Steel, Heat Treatment: 1038°C (1900°F) + Age
Subcategory: Ferrous Metal; Metal; Precipitation Hardening Stainless; Stainless Steel
Key Words: Allvac, an Allegheny Teledyne Company, 17-4PH, 17/4PH, 17-4 PH, AMS 5604, ASTM 240-QQS 766, DIN 1.4542, UNS S17400; PWA 1091. PDS 10705 GD-GF
| Component | Wt. % |  | | | C | 0.035 | | | Cr | 16.3 | | | Cu | 4 | | | Fe | 74 | |
| | Component | Wt. % |  | | | Mn | 0.5 | | | Nb | 0.3 | | | Ni | 4 | |
| | Component | Wt. % |  | | | P | 0.02 | | | S | 0.015 | | | Si | 0.5 | |
|
Material Notes: Iron content calculated as remainder. Data provided by Allvac. Applications: Aircraft and missile fittings, fasteners, gears. Turbine and pump blades, shafts.
| Physical Properties | Metric | English | Comments |
|
| Density | 7.78 g/cc | 0.281 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 351 | 351 | Estimated from Rockwell C value for Brinell test with 3000 kg load/10 mm diameter ball |
| Hardness, Knoop | 382 | 382 | Estimated from Rockwell C value. |
| Hardness, Rockwell C | 38 | 38 | |
| Hardness, Vickers | 367 | 367 | Estimated from Rockwell C value. |
| Tensile Strength, Ultimate | 1172 MPa | 170000 psi | |
| Tensile Strength, Yield | 1069 MPa | 155000 psi | 0.2% Offset |
| Elongation at Break | Min 10 % | Min 10 % | |
| Reduction of Area | Min 40 % | Min 40 % | |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|