Haynes® 230® alloy, as cast vacuum investment casting, tested at 871°C (1600°F)
Subcategory: Metal; Nickel Base; Superalloy
Key Words: UNS N06230, AMS 5878, AMS 5891, DIN 17742 No.2.4733
| Component | Wt. % |  | | | Al | 0.3 | | | B | Max 0.015 | | | C | 0.1 | | | Co | Max 5 | |
| | Component | Wt. % |  | | | Cr | 22 | | | Fe | Max 3 | | | La | 0.02 | | | Mn | 0.5 | |
| | Component | Wt. % |  | | | Mo | 2 | | | Ni | 57 | | | Si | 0.4 | | | W | 14 | |
|
Material Notes: Excellent high-temperature strength, outstanding resistance to oxidizing environments up to 1149°C, premier resistance to nitriding environments, and excellent long-term thermal stability. Applications include combustion cans, transition ducts, flameholders, thermocouple sheaths and other gas turbine components; used for catalyst grid supports in ammonia burners, high-strength thermocouple protection tubes, high-temperature heat exchangers, ducts, high-temperature bellows; furnace retorts, chains and fixtures, burner flame shrouds, recuperator internals, dampers, nitriding furnace internals, heat-treating baskets, grates, trays, sparger tubes, and cyclone internals. Data provided by the manufacturer, Haynes International, Inc.
| Physical Properties | Metric | English | Comments |
|
| Density | 8.97 g/cc | 0.324 lb/in³ | at RT |
Mechanical Properties |
|
| Tensile Strength, Ultimate | 285 MPa | 41300 psi | |
| Tensile Strength, Yield | 185 MPa | 26800 psi | at 0.2% offset |
| Elongation at Break | 19 % | 19 % | in 5D |
| Reduction of Area | 29.8 % | 29.8 % | |
| Modulus of Elasticity | 211 GPa | 30600 ksi | RT |
| Modulus of Elasticity at Elevated Temperature | 150 GPa | 21800 ksi | 1000°C (1830°F) |
| Modulus of Elasticity at Elevated Temperature | 157 GPa | 22800 ksi | 900°C (1650°F) |
| Modulus of Elasticity at Elevated Temperature | 164 GPa | 23800 ksi | 800°C (1470°F) |
| Modulus of Elasticity at Elevated Temperature | 171 GPa | 24800 ksi | 700°C (1290°F) |
| Modulus of Elasticity at Elevated Temperature | 177 GPa | 25700 ksi | 600°C (1110°F) |
| Modulus of Elasticity at Elevated Temperature | 184 GPa | 26700 ksi | 500°C (930°F) |
| Modulus of Elasticity at Elevated Temperature | 190 GPa | 27600 ksi | 400°C (750°F) |
| Modulus of Elasticity at Elevated Temperature | 196 GPa | 28400 ksi | 300°C (570°F) |
| Modulus of Elasticity at Elevated Temperature | 202 GPa | 29300 ksi | 200°C (390°F) |
| Modulus of Elasticity at Elevated Temperature | 207 GPa | 30000 ksi | 100°C (212°F) |
| Charpy Impact | 73 J | 53.8 ft-lb | solution annealed, 41 J after 8000 hours at 650°C (1200°F), 28 J after 8000 hours at 760°C (1400°F), 28 J after 8000 hours at 870°C (1600°F) |
Electrical Properties |
|
| Electrical Resistivity | 0.000125 ohm-cm | 0.000125 ohm-cm | RT |
| Electrical Resistivity at Elevated Temperature | 0.000125 ohm-cm | 0.000125 ohm-cm | 1000°C (1830°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001258 ohm-cm | 0.0001258 ohm-cm | 100°C (212°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001265 ohm-cm | 0.0001265 ohm-cm | 200°C (390°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001271 ohm-cm | 0.0001271 ohm-cm | 900°C (1650°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001273 ohm-cm | 0.0001273 ohm-cm | 300°C (570°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001284 ohm-cm | 0.0001284 ohm-cm | 400°C (750°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001291 ohm-cm | 0.0001291 ohm-cm | 800°C (1470°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001302 ohm-cm | 0.0001302 ohm-cm | 500°C (930°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001307 ohm-cm | 0.0001307 ohm-cm | 700°C (1290°F) |
| Electrical Resistivity at Elevated Temperature | 0.0001312 ohm-cm | 0.0001312 ohm-cm | 600°C (1110°F) |
Thermal Properties |
|
| CTE, linear 20°C | 12.7 µm/m-°C | 7.06 µin/in-°F | 25-100°C (77-212°F) |
| CTE, linear 250°C | 13 µm/m-°C | 7.22 µin/in-°F | 25-200°C (77-390°F) |
| CTE, linear 500°C | 13.3 µm/m-°C | 7.39 µin/in-°F | 25-300°C (77-570°F) |
| CTE, linear 500°C | 13.7 µm/m-°C | 7.61 µin/in-°F | 25-400°C (77-750°F) |
| CTE, linear 500°C | 14 µm/m-°C | 7.78 µin/in-°F | 25-500°C (77-930°F) |
| CTE, linear 1000°C | 14.4 µm/m-°C | 8 µin/in-°F | 25-600°C (77-1110°F) |
| CTE, linear 1000°C | 14.8 µm/m-°C | 8.22 µin/in-°F | 25-700°C (77-1290°F) |
| CTE, linear 1000°C | 15.2 µm/m-°C | 8.44 µin/in-°F | 25-800°C (77-1470°F) |
| CTE, linear 1000°C | 15.7 µm/m-°C | 8.72 µin/in-°F | 25-900°C (77-1650°F) |
| CTE, linear 1000°C | 16.1 µm/m-°C | 8.94 µin/in-°F | 25-1000°C (77-1830°F) |
| Specific Heat Capacity | 0.397 J/g-°C | 0.0949 BTU/lb-°F | RT |
| Specific Heat Capacity at Elevated Temperature | 0.419 J/g-°C | 0.1 BTU/lb-°F | 100°C (212°F) |
| Specific Heat Capacity at Elevated Temperature | 0.435 J/g-°C | 0.104 BTU/lb-°F | 200°C (390°F) |
| Specific Heat Capacity at Elevated Temperature | 0.448 J/g-°C | 0.107 BTU/lb-°F | 300°C (570°F) |
| Specific Heat Capacity at Elevated Temperature | 0.465 J/g-°C | 0.111 BTU/lb-°F | 400°C (750°F) |
| Specific Heat Capacity at Elevated Temperature | 0.473 J/g-°C | 0.113 BTU/lb-°F | 500°C (930°F) |
| Specific Heat Capacity at Elevated Temperature | 0.486 J/g-°C | 0.116 BTU/lb-°F | 600°C (1110°F) |
| Specific Heat Capacity at Elevated Temperature | 0.574 J/g-°C | 0.137 BTU/lb-°F | 700°C (1290°F) |
| Specific Heat Capacity at Elevated Temperature | 0.595 J/g-°C | 0.142 BTU/lb-°F | 800°C (1470°F) |
| Specific Heat Capacity at Elevated Temperature | 0.609 J/g-°C | 0.146 BTU/lb-°F | 900°C (1650°F) |
| Specific Heat Capacity at Elevated Temperature | 0.617 J/g-°C | 0.147 BTU/lb-°F | 1000°C (1830°F) |
| Thermal Conductivity | 8.9 W/m-K | 61.8 BTU-in/hr-ft²-°F | RT |
| Thermal Conductivity at Elevated Temperature | 10.4 W/m-K | 72.2 BTU-in/hr-ft²-°F | 100°C (212°F) |
| Thermal Conductivity at Elevated Temperature | 12.4 W/m-K | 86.1 BTU-in/hr-ft²-°F | 200°C (390°F) |
| Thermal Conductivity at Elevated Temperature | 14.4 W/m-K | 99.9 BTU-in/hr-ft²-°F | 300°C (570°F) |
| Thermal Conductivity at Elevated Temperature | 16.4 W/m-K | 114 BTU-in/hr-ft²-°F | 400°C (750°F) |
| Thermal Conductivity at Elevated Temperature | 18.4 W/m-K | 128 BTU-in/hr-ft²-°F | 500°C (930°F) |
| Thermal Conductivity at Elevated Temperature | 20.4 W/m-K | 142 BTU-in/hr-ft²-°F | 600°C (1110°F) |
| Thermal Conductivity at Elevated Temperature | 22.4 W/m-K | 155 BTU-in/hr-ft²-°F | 700°C (1290°F) |
| Thermal Conductivity at Elevated Temperature | 24.4 W/m-K | 169 BTU-in/hr-ft²-°F | 800°C (1470°F) |
| Thermal Conductivity at Elevated Temperature | 26.4 W/m-K | 183 BTU-in/hr-ft²-°F | 900°C (1650°F) |
| Thermal Conductivity at Elevated Temperature | 28.4 W/m-K | 197 BTU-in/hr-ft²-°F | 1000°C (1830°F) |
| Melting Point | 1301 - 1371 °C | 2370 - 2500 °F | |
| Solidus | 1301 °C | 2370 °F | |
| Liquidus | 1371 °C | 2500 °F | |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. MatWeb data and tools provided by MatWeb, LLC.
|